1 / 18

Review of Zeron ® 100 Failures in Dulang

ADAPTED PRESENTATION Date : 24 November, 2009 (Week 48) Location: PCSB Kerteh HQ. Review of Zeron ® 100 Failures in Dulang. Iain Rei Technical Director. Background. Parties Operator (OC): Petronas Carigali Sdn . Bhd. Service Provider (SP): Geowell Sdn. Bhd.

abril
Télécharger la présentation

Review of Zeron ® 100 Failures in Dulang

An Image/Link below is provided (as is) to download presentation Download Policy: Content on the Website is provided to you AS IS for your information and personal use and may not be sold / licensed / shared on other websites without getting consent from its author. Content is provided to you AS IS for your information and personal use only. Download presentation by click this link. While downloading, if for some reason you are not able to download a presentation, the publisher may have deleted the file from their server. During download, if you can't get a presentation, the file might be deleted by the publisher.

E N D

Presentation Transcript


  1. ADAPTED PRESENTATION Date: 24 November, 2009 (Week 48) Location: PCSB KertehHQ Review of Zeron®100 Failures in Dulang Iain Rei Technical Director

  2. Background • Parties • Operator (OC): PetronasCarigaliSdn. Bhd. • Service Provider (SP): Geowell Sdn. Bhd. • Wire Supplier (WS): Wilco OFS Pte. Ltd. • Location: Dulang, PMO • Scope of Work • SP to provide sand-bailing services • WS to provide super-duplex stainless steel Zeron®100 HS

  3. Background: Timeline • Timeline • First contact: Week 40 (Susp. wire thinning) • KSB Visit: Week 41 (Wire inspection) • Second Contact: Week 42 (Susp. Inconsistent OD) • KSB Visit: Week 43 (Wire inspection) • Wire replacement: Week 43 (Inconclusive) • Official reply: Week 45 (Mfg. Tolerance) • Third Contact: Week 47 (Susp. lower MBL; surface quality; plastic behavior) • KSB Visit: Week 48 (now)

  4. Background: Zeron®100 • First used in Dulang: 2003 • SP: Dimension Bid Sdn. Bhd. • Current countries: 6 • Malaysia, Indonesia, Vietnam, Thailand, Myanmar, Turkmenistan • Current mean per annum usage: 60 reels • Largest end-user: PetronasCarigali • Largest single-user: Chevron Thailand • Keywords: high breaking load, quality, consistency, support, service, stockist, fast

  5. Background: Zeron®100

  6. Discussion: Thinning • First issue: Wire thinning • Restatement: wire is surface thinning inexplicably causing disruption in service • Premise: • Wire was said to be unused and new from reel • Wire was of poor surface quality • Conclusion: • Wire was found to be used • Wire was found to be significantly stressed mechanically • Link to reportfrom UK

  7. Discussion: Thinning

  8. Discussion: OD • Second issue: Inconsistent OD • Restatement: wire OD is inconsistently thick or thin, resulting in uncertainty in quality that could lead to NPT • Premise: • Wire is said to be new • Wire OD was changing rapidly during spooling • Operator/helper detected accurately using hands on moving wire from supply to usage reel • Conclusion: • Wire is new • Wire OD seemed to be changing if detected by hand • Wire was replaced • Subsequent findings from Principal show that OD was fluctuating within normal manufacturing limits of ±0.001” 

  9. Discussion: OD • Our findings • On 23 Nov., 2009 we performed a series of measurements on a reel that is supposedly problematic with an undulating OD. • Using an electronic caliper provided by Geowell, we conducted a series of measurements of theOD of the wire • The result is an OD measurement of 0.108”±0.00045”ora breaking load of 2,500lb±25.21lb • Error is within manufacturing error of 0.001”

  10. Discussion: Plasticity • Third issue: Plastic behavior of Zeron®100 wire • Restatement: wire elongates without recovering original length on tension; indication of poor quality • Premise: • Break load testing methods are normal and common; equipment used to test is approved • Wire elongates plastically without returning to original length under load • Conclusion: • Tested wire had already broken at rope socket but was undiscovered • Subsequent “elongation” was due to wire being pulled out of rope socket • Cup-cone break-ends of wire indicates wire is of good quality 

  11. Discussion: Plasticity What is elasticity and plasticity? • Elasticity: when a material behaves elastically like rubber • On tension an elastic material will elongate proportionately with tension • On release of tension, an elastic material will retain its original length • Plasticity: when a material does not behave elastically • On tension beyond the elastic limit, a material will begin to act plastically • The subsequent increase in tension will not result in proportional elongation of length • On release of tension, the material will not return to its original length Plastic return of length Δx (plastic elongation)

  12. Discussion: Plasticity

  13. Summary • Findings • Most findings conclusively attest to the quality of Zeron®100 • Thinning on recent sand bailing activity is not yet examined and as yet outside of our scope of control • Thinning is akin to mechanical erosionwhereas stress-corrosion-cracking is a form of chemical erosion (or commonly called corrosion) • Problems that have occurred to not seem to be due to the quality of the material or drawn wire 

  14. Summary • Recommendations • Shorter runs-between-cut/test cycles • Closer surface inspection for scratches and large reductions in OD of wire between run-cycles • Wilco have been recommended to: • Check for well schematic • Check for nipple or SSD profiles, kick-offs, deviation angles, etc. that may lead to high forces of friction • Request more supporting information from OC and SP • Provide continued support to OC and SP

  15. Case Study • Example: Chevron wire thinning • WI/125xx; max pull: 1,350lb; on reel: 21,115'; 271 runs • Mobilized in November 2007 • 25,000ft ZERON®100, 0.125” • WI/125xx; max pull: 1,500lb; on reel: 18,545'; 258 runs • Mobilized in March 2009 • 20,000ft ZERON®100, 0.125”

  16. Case Study • Example: Chevron wire thinning • Chevron runs in the northern and southern offshore fields • 20,000+ runs per year • Typical measured depth of wells: 14,000-16,000ft • Typical ordered slickline: ZERON®100, 0.125” • Typical ordered length: 20,000ft • Typical service company junk length: Remaining on drum ≥ 1.5 x Well MD • Shows great belief in their program and our wire

  17. Wilco Website Preview • Surface information • History • Work history • Technical information • Material data sheets • Test certificates (private access) • FirstLook Calculator • Contact point « http://www.wilcowirelines.com »

  18. Contact Us Wilco Oilfield Services Pte. Ltd. (estd. 1982) No. 9, Kaki Bukit Road 3, East Point Terrace, Singapore 417829 Tel: +65(6)482-3666; Fax: +65(6)482-4782 Visit us at: www.wilcowirelines.com Email us: wilco@wilcowirelines.com For a full technical presentation, please contact us. Focus group: well & production engineers

More Related