An Image/Link below is provided (as is) to download presentation Download Policy: Content on the Website is provided to you AS IS for your information and personal use and may not be sold / licensed / shared on other websites without getting consent from its author. Content is provided to you AS IS for your information and personal use only. Download presentation by click this link. While downloading, if for some reason you are not able to download a presentation, the publisher may have deleted the file from their server. During download, if you can't get a presentation, the file might be deleted by the publisher.

E N D

Presentation Transcript


  1. Stress Corrosion Cracking of Stainless Steels in High Pressure Alkaline Electrolysers HySafe conference, Pisa 2005-09-08 Kristian Haraldsen and Håkon Leth-Olsen, Norsk Hydro ASA, Corporate Research Centre

  2. Content • Background • Stress Corrosion Cracking (SCC) • SCC in Alkaline environments • Experimental setup • Materials • Test conditions • Results • Austenitic stainless steels • Duplex stainless steels • Welded Duplex stainless steels • Conclusions and recommendations

  3. Background • Atmospheric electrolysers operate safely with austenitic stainless steel of type AISI 316L or similar. • Newly developed high pressure electrolysers operate at 70 – 80°C with 30 – 40% KOH solution and an O2 pressure of 15 – 30 bar. • A few occasions of leakages have been observed at the oxygen side of high pressure electrolysers. • Construction material AISI 316L • Located in weld or close to the weld (heat affected zone – HAZ) • Confirmed to be intercrystalline stress corrosion cracking (SCC) • Commonly referred SCC temperature limit for AISI 316L in high concentrated caustic solution is about 100°C • Need for alternative materials for safe use in high pressure electrolysers • Nickel base alloys resistant, but high price materials

  4. Examples of leaks Separator lye Penetrant

  5. Stress Corrosion Cracking (SCC) • Failure of engineering materials by slow, environmentally induced crack propagation • Combined effect of tensile stresses and corrosion reactions • Tensile stresses • Externally applied loads (static) • Residual stresses from welding, machining etc. • May occur in materials resistant to general corrosion in the same environment • Initiates at local defects in oxide layer • Difficult to predict and identify before leakage • No fore-warning • NDT (non-destructive testing) methods not very informative • Inspection in small size piping difficult Tensile stresses Environ- ment Material SCC

  6. SCC in Alkaline Environments • Commonly referred temperature limit for AISI 316L in high concentrated caustic solution is 100°C • Temperature limit lowered by the high oxygen pressure • Oxidising conditions may cause trans-passive dissolution of Cr as CrVI

  7. Experimental • Resistance to SCC tested by autoclave exposure of C-ring specimens • Test specimens tensioned to plastic deformation • Test conditions: • Solution: 30 and 40% KOH • Temperature: 90, 100 and 120°C • Oxygen pressure: 15 and 30 bar • Exposure time: 3 months • Results analysed by • Visual examination • Optical microscopy • Scanning electron microscopy (SEM) • General corrosion by weight-loss

  8. Materials • Materials selected based on expected resistance, availability and price. • Stainless steels with increased nickel (Ni) and chromium (Cr) content • Duplex stainless steels

  9. Results – Austenitic stainless steels • Susceptibility of AISI 316L/Ti confirmed, SCC at 100°C, 40% KOH and 30 bar O2 • Bolts of AISI 316L (A4) fractured at 90°C, 30% KOH and 15 bar O2 (SCC) • 2RE10 (AISI 310L): SCC at 100 °C, 40% KOH and 30 bar O2

  10. Results – Austenitic stainless steels (continue) • 2RK65 (904L): SCC at 100 and 120 °C, 40% KOH and 30 bar O2 • Alloy 28 showed no cracking at 90°C, 30% KOH and 15 bar O2

  11. Results – Duplex stainless steels • Duplex 2507: SCC at 100 °C, 40% KOH and 30 bar O2 • Duplex 2304: no SCC at 100 and 120°C , 40% KOH and 30 bar O2 • General corrosion attacs occurred at 120°C

  12. Results – Duplex stainless steels (continue) • Duplex 2906 showed cracking at 120°C, 40% KOH and 30 bar O2 • Duplex 2205 showed no cracking at 100°C, 40% KOH and 30 bar O2

  13. Welded Duplex 2205 • Duplex 2205 chosen for further qualification • Good resistance to SCC • Rel. low Price, good availability • Need to test welded specimens • Welding procedure of duplex stainless steels important • SCC often occur in connection with welds • Welded C-ring test specimens prepared • Tested at 100 and 120°C, 40% KOH and 30 bar O2 • Both tensioned and relaxed weld area • Weight loss coupons for general corrosion rate • Repeated test of base material

  14. Welded Duplex 2205 - results • General corrosion rate: • 0.1 mm/year at 100°C • 0.6 mm/year at 120°C • No SCC found in base material or in connection with relaxed welds • SCC occurred in tensioned weld at 100°C • Metallographic analyses did not reveal any deviance of the weld • No cracking in HAZ • No SCC in tensioned weld at 120°C • Protected by high general corrosion rate • Repeated tests did not reveal any SCC in the weld or base material

  15. Duplex 2205 with alternative welds • Duplex 2205 with alternative weld filler materials tested at 100°C: • Nickel base alloy 600 (18-22% Cr, >67% Ni) • Nickel base alloy 625 (22% Cr, 64.5% Ni, 9% Mo) • No SCC occurred • Limited localised corrosion • Located inHAZ • 50-100 µm deep (0.2-0.4 mm/y) • Local/general corrosion rate • Dependent on temperature • Expected to be lower at 70 - 80°C • Further testing needed

  16. Summary of test results ** General corrosion attacks *** Local corrosion attacks * Bolt of AISI 316L broke

  17. Summary and Conclusions • Austenitic stainless steels vulnerable to SCC on oxygen side of high-pressure alkaline electrolysers at elevated temperatures • Alternatives • Use of alloy 28 (if available) • Use of Duplex 2205 with increased temperature safety limit • Special focus on weld procedure (max. temperature) • Use of Duplex 2205 with nickel base alloy weld filler material • Further qualification with regards to localised corrosion needed • Nickel base alloys in vulnerable pipes • Non-welded connections (without residual tensile stresses) • Practical modifications • Duplex 2205 piping with non-welded connections • Welded Duplex 2205 in tanks • Decreased temperature from 80°C to 60°C.