1 / 31

Polymers - process & post-processing treatments induced failures

Polymers - process & post-processing treatments induced failures. Dr Xi Peng Polymer Scientist. Agenda. Polymer and Plastics Product Concept Plastics Processing and Issues Post-processing Treatment Testing and Problem Solving. Polymer and Plastics. Polymer

zazu
Télécharger la présentation

Polymers - process & post-processing treatments induced failures

An Image/Link below is provided (as is) to download presentation Download Policy: Content on the Website is provided to you AS IS for your information and personal use and may not be sold / licensed / shared on other websites without getting consent from its author. Content is provided to you AS IS for your information and personal use only. Download presentation by click this link. While downloading, if for some reason you are not able to download a presentation, the publisher may have deleted the file from their server. During download, if you can't get a presentation, the file might be deleted by the publisher.

E N D

Presentation Transcript


  1. Polymers - process & post-processing treatments induced failures Dr Xi Peng Polymer Scientist

  2. Agenda • Polymer and Plastics • Product Concept • Plastics Processing and Issues • Post-processing Treatment • Testing and Problem Solving

  3. Polymer and Plastics • Polymer • A polymer is a long chain of small molecules repeatedly joined together • Plastics • A plastic is a mixture of a polymer material and additives (anti-oxidants, fillers, plasticisers, pigments, UV stabilisers, etc..) Polyethylene (PE)

  4. Product Concept • Material Selection • Design • In-service Conditions • Processing

  5. Material Selection There are approximately 100 generic types of plastic e.g. polypropylene, Nylon, phenolic resin. Within these types are subgroups e.g. Nylon: Nylon 6, Nylon 6-6, Nylon 12 For each subgroup there will be many grades available: e.g. easy flow, food grade, UV stabilised, fire retardant, etc.

  6. Influences of Design • Item size • Assembly methods (e.g. screw fixing, welding, adhesives, snap fitting, etc.) • Transparency • Surface finish • In contact with other materials • Expected life • End of life – recycling, biodegradable

  7. In-service Conditions • Temperature requirements – minimum/maximum temperature; continuous or occasional exposure • Chemicals from surroundings • Stress – residual stress from moulding; stress from assembly method; applied stress in the application • Outdoor application – UV resistance • Fire retardant • Electrical properties

  8. Plastics Processing • Moulding - Injection, Blow, Transfer, Rotational • Extrusion - Continuous long items of uniform section, e.g. film, sheet, pipe, profile, coating • Forming - Vacuum Forming, Pressure Forming • Other - Spreading, Dipping, Sintering, Casting

  9. Plastics Processing • Extrusion – Film • Extrusion – Pipe • Extrusion – Profile • Other Extrusion • Injection Moulding • Blow Moulding • Thermoforming • Other Processes SmithersRapra

  10. Injection Moulding • Probably the most common plastic processing technique • Rapid cycle time with good dimensional control & part to part consistency • Materials must be well mixed to ensure uniform melting • Items can be identified by the marks of gate & ejector pins

  11. Injection Moulding Common Issues: • Short shot – incomplete mould filling • Flashing – leakage of molten plastic around split line or core pins • Weld lines – poor weld line strength • Sinking & Voiding • Poor dimensional tolerances • Warpage • Excessive residual stresses • Brittle mouldings

  12. Extrusion • Continuous long items of uniform section • Rods & tubes • Gas & water pipes • Window frames • Cable sheathing • Films & Sheets • Compounding of filled or reinforced grades of plastic materials

  13. Extrusion Common Issues: • Contamination • Polymer chain scission & cross-linking • Surface instability – sharkskin • Cooling rate control • Co-extrusion problems • Uneven mixing in compounding

  14. Post-processing Treatment One-off Process • Annealing – heating plastic part at an temperature close to its Tgthat makes the residual stresses relieved and increases its ductility • Machining – controlled material-removal process in which a component is cut, drilled or polished into a desired final shape and size • Coating – a process of applying covering to the surface of an object for decorative and/or functional purposes

  15. Post-processing Treatment contd. Multiple Repeat Process • Cleaning – a process using devices and cleaning agents to clean items • Sterilisation – any process that eliminates microbiological organisms present on the surface of device

  16. Cleaning • To remove any unwanted substances – the contaminations from the part surface • May involve heat, pressure & chemicals • Cleanliness validation – surface analysis

  17. Issues Caused by Cleaning Process • Degradation – can be caused by heat (thermal oxidation), chemical attack and/or hydrolysis; leading to reduction of molecular weight and deterioration of the physical/chemical properties • Material migration – relates to low molecular weight species present in plastics, e.g. residual monomers, additives, low molecular weight oligomers, reaction/breakdown products, etc.; migration increased due to heat and/or polymer swelling

  18. Issues Caused by Cleaning Process • Environmental stress cracking (ESC) – exposed to chemical environment in combination with tensile stress • Delamination – co-extruded or over-moulded items; thermal expansion of polymer ~ 10 times metal insert • Discolouration – yellowing due to generation of coloured species during degradation

  19. Sterilisation Main methods: • Heat (e.g. dry, steam, boiling) • Pressure (e.g. autoclave) • Chemicals (e.g. ethylene oxide) • Ionising radiation (e.g. Gamma rays, electron beam) Effects on polymers vary depending on the polymer structure

  20. Issues Caused by Sterilisation Process • Degradation leading to polymer chain scission and/or cross-linking • Change in colour – e.g. yellowing • Generation of odour due to volatiles formed by reactions • Leave toxic residuals or by-products on the polymer surface • Influence on extractables and leachables • Disintegration of multi-layer and over-moulded part

  21. Analysis Techniques for Process-Induced Failures Polymer Degradation • Gel permeation chromatography (GPC): measurement of molecular weight (MW) and molecular weight distribution • Rheological testing: e.g. melt flow index (MFI), rotational viscometry • Mechanical testing: e.g. tensile strength and modulus, elongation

  22. Analysis Techniques for Process-Induced Failures Contamination • Infrared spectroscopy (FT-IR): identification of polymers & contaminants • Microscopy combined with elemental analysis technique (e.g. scanning electron microscopy/energy dispersive X-ray analysis, SEM/EDX): detection & identification of any inclusions and unspecified materials • Chromatography (e.g. gas chromatography with mass spectrometry, GC-MS): separation & identification of low molecular weight contaminants

  23. Analysis Techniques for Process-Induced Failures Porosity & Voids – may cause structural weakness & stress concentration • Optical and/or electron microscopy (e.g. SEM) • Pressure leak testing

  24. Analysis Techniques for Process-Induced Failures Excessive Residual Stresses – may cause environmental stress cracking (ESC) • Dip testing: by applying a known ESC agent (solvent) to the part any high stress areas will tend to crack; the time-to-crack is indicative of the level of residual stress • Thermal analysis (e.g. differential scanning calorimetry, DSC): indication of processing history that determines the level of residual stress • Impact test: high residual stress low impact strength

  25. Analysis Techniques for Process-Induced Failures Uneven Mixing of Components – may cause structural weakness & stress concentration • Optical and/or electron microscopy (e.g. SEM) • Thermal analysis (e.g. thermogravimetric analysis, TGA): providing information about additives/fillers

  26. Analysis Techniques for Process-Induced Failures Low or Excessive Crystallinity high crystallinityembrittlement low crystallinity loss of properties • X-ray diffraction (XRD): determination of crystallinity and crystallite size • Thermal analysis (e.g. differential scanning calorimetry, DSC): providing information about relative crystallinity

  27. Analysis Techniques for Process-Induced Failures Material Migration Can alter the extractables and leachables profile – generally include processing aids, polymerisation residues, additives & reaction products • Profiling of chemical species by GC-MS • Identifies relatively volatile, thermally stable compounds • Molecular weight range 50 to~500 Daltons

  28. Material Migration contd. • Profiling of chemical species by LC(liquid chromatography)-MS • Identifies volatile to oligomeric sized compounds • Can be used for thermally unstable compounds, polar compounds and aromatic hydrocarbons • Molecular weight range 200 to >1000 Daltons • Quantitative determination of trace elements by inductively coupled plasma (ICP) • Quantitative determination of non-volatile residues (NVR) • Infrared (FT-IR) analysis of NVR – overall chemical nature of residues

  29. Summary